Thermoplastic Elastomer (TPE) delivers the soft, rubber-like feel of vulcanized rubber while processing like a standard thermoplastic. It offers an adjustable hardness from Shore A 20 to 90, excellent grip, and the ability to be overmolded directly onto rigid substrates such as PP, PC, and ABS. Shinzoft provides OEM/ODM TPE injection molding and two-shot overmolding for tool grips, toothbrush handles, seals, and soft-touch buttons, from DFM through mass production.
TPE recreates rubber's softness and rebound but can be injection molded, extruded, and reground. Scrap and runners return to the machine instead of becoming waste, unlike thermoset rubber that is permanently crosslinked.
Grades span Shore A 20 (very soft, seal-like) to Shore A 90 (firm, wear-resistant). One part design can be tuned across a wide feel range by selecting a different durometer.
TPE bonds chemically to rigid substrates during molding. PP gives the strongest adhesion; ABS, PC, and PA also bond well with the right grade or primer. This produces permanently attached soft grips without adhesive.
A high coefficient of friction and comfortable matte feel make TPE the default choice for handheld products. Mold texture can be tuned from smooth to leather-like, adding grip without changing the material.
Values below cover the common styrenic (SEBS-based) TPE-S family at a mid-range hardness of about Shore A 60. Property values shift with hardness, base chemistry, and oil content.
| Property | Typical Value | Notes |
|---|---|---|
| Density | 0.90–1.20 g/cm³ | Some grades float; rises with filler content |
| Tensile Strength | 5–12 MPa | Lower than rigid plastics; elongation often exceeds 500% |
| Hardness Range | Shore A 20–90 | Single family spans seal-soft to fairly firm |
| Heat Deflection Temp (HDT, 1.8 MPa) | 60–90 °C | Limited upper temperature; grade-dependent |
| Service Temperature Range | −40 to +90 °C | Stays flexible at low temperature |
| Molding Shrinkage | 0.8–2.5 % | Varies with hardness and wall thickness |
| Volume Resistivity | 10¹³–10¹⁵ Ω·cm | Good insulator; antistatic grades available |
| Parameter | Typical Range |
|---|---|
| Drying Temperature / Time | Usually not required; 80 °C / 2–3 h for moisture-sensitive grades |
| Melt Temperature | 180–230 °C |
| Mold Temperature | 20–50 °C |
| Injection Pressure | 40–80 MPa |
| Typical Cycle Time | 15–45 s, depending on wall thickness |
TPE processes easily on standard machines, but a few details decide quality. Keep melt temperature stable and moderate: too hot and the low-viscosity melt sticks to the mold or degrades, too cold and flow lines appear. Avoid sharp gates and dead zones in the runner because they shear the melt and leave marks. For overmolding, the substrate must be clean and molded from a compatible grade — PP gives the strongest bond, while other substrates may need a primer. Cooling is fast at low mold temperature, but soft parts need gentle ejection to avoid tearing, and thick sections fill best at lower injection speed to prevent sink marks.
TPE's closest relatives are the other soft materials. Compared with TPU, TPE is softer, cheaper, and easier to mold, but TPU wins decisively on abrasion resistance, oil resistance, and elastic recovery. Where a soft grip or a mild seal is the goal, TPE is often the economical choice; where the part rubs against rough surfaces or contacts oils, TPU lasts longer.
Against PVC, TPE offers a cleaner rubber feel, better aging, and no plasticizer migration, while flexible PVC stays cheaper and inherently flame retardant. TPE also overmolds onto rigid PP more reliably than most alternatives, which is why PP plus TPE is the standard pairing for two-shot tool handles.
TPE is the broad family of thermoplastic elastomers. TPU is a specific, high-performance type known for abrasion and oil resistance, while TPR usually refers to styrenic TPE-S compounds used in softer consumer parts. TPR often means the same SEBS-based material as TPE, and the naming varies by supplier.
Yes, and this is one of TPE's main strengths. It bonds chemically to rigid substrates during the molding cycle, with no adhesive. PP gives the strongest bond; ABS, PC, and PA also bond well when paired with a compatible grade or a primer. The result is a permanent soft grip that resists peeling.
Match hardness to function. Shore A 20–40 suits very soft seals and cushions, Shore A 50–70 covers most grips and soft-touch surfaces, and Shore A 80–90 gives a firm, wear-resistant feel for structural overmolds. Because the family shares one processing method, changing durometer rarely changes the part design.
Yes, provided the correct grade is specified. Food-contact and medical grades of TPE are available and meet FDA, USP Class VI, and ISO 10993 requirements depending on the application. We mold these only with certified compounds, on dedicated and cleaned equipment.
In many soft-touch, grip, and sealing applications, yes. TPE is easier to process, regrind and remold, and costs less than silicone. Silicone still leads where extreme temperature resistance from −60 °C to 200 °C, optical clarity, or a very inert surface is required. For most consumer grips and seals, TPE does the job at lower cost.
Send your drawings, substrate material, and target feel. Our engineers will recommend the right TPE grade and durometer and deliver clean, repeatable overmolded parts.
Shinzoft serves customers worldwide with custom TPE injection molding solutions and a full range of injection molding materials.
Get a Free Quote →