HDPE (High-Density Polyethylene) is a semi-crystalline thermoplastic with a density of 0.941–0.965 g/cm³, known for its stiffness, outstanding chemical resistance, and low-temperature impact strength that stays intact below −60 °C. It is the workhorse material for industrial containers, pipe fittings, crates, outdoor equipment housings, and toys. Shinzoft provides full-service OEM/ODM HDPE injection molding from DFM and tooling through validated mass production.
Higher crystallinity than LDPE gives HDPE a tensile strength of 20–30 MPa and a flexural modulus around 1,000–1,400 MPa, so large parts hold their shape under stacked loads without extra ribs or metal inserts.
HDPE resists acids, alkalis, salts, alcohols, and most detergents, with water absorption below 0.01%. It is the standard choice for chemical-contact parts and washdown environments.
Brittleness temperature sits below −60 °C. Notched Izod impact values of 100–400 J/m mean outdoor parts keep performing in freezing conditions where PP or PS would crack.
Molding shrinkage of 1.5–4% is large and directional. In thick or heavily ribbed parts this drives warpage, so gate position and cooling layout must be designed around the flow direction of the melt.
Values below reflect unfilled, general-purpose injection molding grades. The wide shrinkage range is a direct result of density and crystallinity, so always confirm with your specific grade data sheet.
| Property | Typical Value | Notes |
|---|---|---|
| Density | 0.941–0.965 g/cm³ | Higher density means higher crystallinity and stiffness |
| Tensile Strength (Yield) | 20–30 MPa | Varies strongly with density and comonomer content |
| Flexural Modulus | 1,000–1,400 MPa | Rigid enough for structural crates and containers |
| Elongation at Break | >500% | Highly ductile, absorbs impact by deformation |
| Heat Deflection Temp (HDT, 1.8 MPa) | 60–80 °C | Not for high-temperature service above ~80 °C |
| Melting Point | 125–135 °C | Semi-crystalline; sharp melting transition |
| Molding Shrinkage | 1.5–4.0 % | Directional; plan for warpage in long flat parts |
| Water Absorption | <0.01 % | Essentially non-hygroscopic, no drying needed |
| Dielectric Strength | 18–22 kV/mm | Good insulation for electrical housings |
| Parameter | Typical Range |
|---|---|
| Drying Temperature / Time | Not required (non-hygroscopic; keep pellets clean and dry) |
| Melt Temperature | 200–260 °C |
| Mold Temperature | 20–60 °C |
| Injection Pressure | 70–120 MPa |
| Holding Pressure | 40–70 MPa (higher to offset large shrinkage) |
| Typical Cycle Time | 20–60 s (depends on wall thickness) |
HDPE has a broad processing window and forgives moderate parameter drift, but the large, directional shrinkage is where most problems originate. Run higher hold pressure and longer hold time than you would for PP, and favor generous cooling on thick sections. Because the melt is non-hygroscopic, drying is unnecessary — but pellets should still be stored clean to avoid splay and contamination defects.
HDPE sits at the stiff, strong end of the polyethylene family. Against LDPE, it delivers roughly double the stiffness and better load-bearing, at the cost of softness and clarity — LDPE wins for squeeze-to-dispense parts and soft snap lids. Against LLDPE, HDPE still leads on rigidity and chemical resistance, while LLDPE brings higher tensile toughness, puncture resistance, and better environmental stress crack resistance in thin sections. Compared with PP, HDPE is tougher at low temperature and more resistant to chemicals, but PP is lighter, stiffer above 80 °C, and far better for living hinges.
Plan for 1.5–4.0%, and treat it as directional rather than a single number. Flow-direction shrinkage is lower than cross-flow shrinkage, and higher density grades shrink more. We build the tool with this range in mind and leave steel for adjustment if the first sample needs correction.
No. HDPE is non-hygroscopic with water absorption below 0.01%, so drying is not required. The exception is pellets that have been stored in a humid or cold environment and picked up surface condensation; a short low-temperature dry will clear that and prevent splay marks.
Warpage comes from uneven cooling and directional shrinkage, not from the material itself. Keep wall thickness uniform, place gates so flow paths stay balanced, cool both halves of the tool symmetrically, and use enough hold pressure. A mold flow study before cutting steel is the cheapest way to avoid this.
HDT at 1.8 MPa is roughly 60–80 °C, and the melting point falls between 125–135 °C. Continuous service is normally kept under about 80 °C. On the cold side HDPE is far stronger, staying impact-resistant below −60 °C, which is why it is specified for freezer and outdoor winter applications.
Not reliably in its as-molded state. HDPE has very low surface energy, so inks, labels, and adhesives do not wet the surface well. Corona, flame, or plasma treatment raises the surface energy enough for printing and bonding. If treatment is not practical, design for mechanical fastening, ultrasonic welding, or snap-fits instead.
Upload your drawings and get a quote with a free DFM analysis covering shrinkage direction, gate placement, and warpage risk.
Shinzoft serves customers worldwide with custom HDPE injection molding solutions, and you can review our full range on the materials page.
Get a Free Quote →